Performance ( Alloy ) | 310 | 304 | 430 | 446 |
Melting point range ℃ | 1400-1450 | 1400-1425 | 1425-1510 | 1425-1510 |
Elastic modulus at 870℃ | 12.4 | 12.4 | 8.27 | 9.65 |
Tensile Strength at 870℃ | 152 | 124 | 46.9 | 52.7 |
Expansile modulus at 870℃ | 18.58 | 20.15 | 13.68 | 13.14 |
Conductivity at 500℃ w/m.k | 18.7 | 21.5 | 24.4 | 24.4 |
Gravity at normal temperature g/cm3 | 8 | 8 | 7.8 | 7.5 |
Weight loss after 1000hrs of cyclic oxidation % | 13 | 70(100h) | 70(100h) | 4 |
Sharp cycling of air, Oxidation temperature ℃ | 1035 | 870 | 870 | 1175 |
1150 | 925 | 815 | 1095 |
Corrosion Rate in H2S mil/yr | 100 | 200 | 200 | 100 |
Maximum recommended temperature in SO2 | 1050 | 800 | 800 | 1025 |
Corrosive ratio in natural gas at 815℃ mil/yr | 3 | | 12 | 4 |
Corrosive ratio in coal gas at 982℃ mil/yr | 25 | 225 | 236 | 14 |
Nitridation rate in anhydrous ammonia at 525 ℃ mil/yr | 55 | 80 | <304#>446# | 175 |
Corrosive ratio in CH2 at 454 ℃ mil/yr | 2.3 | 48 | 21.9 | 8.7 |
Carbon increment of alloy at 982℃,25hrs,40cycles % | 0.02 | 1.4 | 1.03 | 0.07 |